Designation acc. to EN 573-3
Abbreviation
State
Mechanical Properties
Rm (MPa)
Rp0,2 (MPa)
A5 (%)
EN AW-1050A
EN AW - Al 99,5
Soft annealed
70
45
40
Impact extruded
130
110
6
EN AW-1070A
EN AW - Al 99,7
Soft annealed
60
18
40
Impact extruded
120
100
4
EN AW-1200
EN AW - Al 99,0
Soft annealed
70
45
40
Impact extruded
130
110
6
EN AW-2017A
EN AW - AlCu4MgSi
Solution annealed and naturally aged
400
350
10
EN AW-5005A
EN AW - AlMn1
Soft annealed
90
35
24
Impact extruded
170
145
4
EN AW-5754
EN AW - AlMg3
Soft annealed
190
80
20
Impact extruded
265
215
4
EN AW-6060
EN AW – AlMgSi
Solution annealed and artificially aged
245
195
10
EN AW-6061
EN AW - AlMg1SiCu
Impact extruded
Solution annealed and artificially aged
EN AW-6082
EN AW - Al Si1MgMn
Impact extruded
190
170
4
Solution annealed and artificially aged
310
260
10
EN AW-7020
EN AW -
Solution annealed and artificially aged
350
290
10
EN AW-7022
EN AW - AlZn5Mg3CuSolution annealed and artificially aged
500
450
7
4047铝合金化学成分
铝AL:余量
锌Zn:≤0.20
锰Mn:≤0.15
镁Mg:≤0.10
铁Fe:≤0.8
硅Si:11.0-13.0
钛Ti:/
铬Cr:/
铜Cu:≤0.30
其它:单个:≤0.05
合计:≤0.15
抗拉强度135-155MPa,延伸率2-4%,布氏硬度50HBS
材料性能
4000系铝合金(Al-Si系)典型代表为4043、4343铝合金,专门做为焊接材料。
4043铝合金具有熔点低、流动性好、耐蚀性好等特点,对避免焊接裂纹十分有利。
4343铝合金比4043铝合金的Si含量高些,具有熔点低、凝固的范围窄、流动性好等特色,有利于焊缝凝固时的补缩踏减少裂纹,用作复合钎焊板包覆层。
表面质量要求:
1、表面不允许有裂纹、腐蚀斑点和硝盐痕迹。
2、表面上允许有深度不超过缺陷所在部位壁厚公称尺寸8%的起皮、气泡、表面粗超和局部机械损伤,但缺陷大深度不能超过0.5mm,缺陷总面积不超过板材总面积的5%。
3、允许供货方沿型材纵向打光至表面光滑。
4、其他要求:有需求方和供货方自己拟定。
标准:
铝板带国家标准(GB/T 3880-2006),适用于铝合金板带材料的统一标准。
联系方式:
联 系 人:唐先生 (销售部 经理)
电 话:0769-87737075 18820607173
地 址:中国 广东 东莞市 东莞市清溪镇青皇工业区
公司主页:https://xttzjs.1688.com/